ASTM A358 Stainless Steel Pipe: The Five Classes, Explained Correctly

ASTM A358/A358M is the specification that governs electric-fusion-welded (EFW) austenitic stainless steel pipe for corrosive service, high-temperature service, or general applications. It is the standard behind most large-diameter stainless pipe on real projects — desalination trains, FGD ducting, column shells, high-temperature headers — because it is written around plate-formed, longitudinally welded cylinders rather than mill-rolled seamless or continuous-welded product.

It is also the most frequently misread stainless pipe standard in circulation. The five classes are not a quality ladder from “basic” to “best”. They describe two independent variables: whether the pipe is single-welded or double-welded, and whether the weld is fully radiographed, spot radiographed, or not radiographed at all. Get those two axes wrong on a purchase order and you will receive pipe that is compliant with a class you did not ask for.

What ASTM A358 actually covers

Per Section 1 of the specification:

  • Product: electric-fusion-welded austenitic chromium-nickel stainless steel pipe, for corrosive service, high-temperature service, or both, or general applications.
  • Grades: nineteen alloy grades are listed in Table 1, with plate chemistry taken from ASTM A240/A240M. Common ones in practice are 304/304L, 316/316L, 321/321H, 347/347H, 309, 310, and duplex grades where the purchaser specifies them.
  • Size: the standard places no restriction on size, but commercial practice is commonly limited to NPS 8 and larger. This is why A358 is the natural home for large-diameter and heavy-wall work.
  • General requirements: material furnished to A358 must also conform to ASTM A999/A999M unless stated otherwise.
  • Supplementary requirements: S1 through S6 are optional and must be called out on the order if you want them — they do not apply automatically.

The five classes: what the standard actually says

The definitions below are taken directly from Section 1.3 of A358/A358M. Read them closely, because most online summaries get them backwards.

ClassWeld constructionFiller metalRadiography
Class 1Double weldedIn all passesCompletely radiographed
Class 2Double weldedIn all passesNo radiography required
Class 3Single weldedIn all passesCompletely radiographed
Class 4Single weldedIn all passes, except the weld pass exposed to the inside surface may be made without filler metalCompletely radiographed
Class 5Double weldedIn all passesSpot radiographed

The mistake that shows up on almost every supplier page

A widely repeated summary states that Class 1 is “single-welded, 100% RT” and Class 3 is “double-welded, 100% RT”, and that Class 5 is an autogenous weld with no filler metal. All three of those statements contradict the specification text:

  • Class 1 is double welded with filler metal in all passes, fully radiographed. It is not single-welded.
  • Class 3 is single welded with filler metal in all passes, fully radiographed. It is not double-welded.
  • Class 5 is double welded with filler metal in all passes, spot radiographed. It is not an autogenous, filler-free weld. Autogenous welding does appear in the specification — but only as the permitted exception for the inside pass of Class 4, under 6.2.2.1 and 6.2.2.2.

If a quotation or a data sheet tells you Class 1 is single-welded, the document was not written against the standard. Ask for the clause reference.

Radiographic requirements, clause by clause

RequirementClassRule
Complete radiographyClass 1, 3, 4All welded joints examined by radiography (clause 16.1)
Spot radiographyClass 5Not less than 12 in. [300 mm] of radiograph per 50 ft [15 m] of weld (clause 16.2)
No radiographyClass 2No radiographic examination required
Acceptance criteriaClass 1, 3, 4ASME BPVC Section VIII, Div. 1, UW-51
Acceptance criteriaClass 5ASME BPVC Section VIII, Div. 1, UW-52
SequencingAllRadiography is permitted before heat treatment (clause 16.5)

Two consequences are worth spelling out for buyers. First, “spot radiographed” is a defined coverage rate, not a discretionary one — 300 mm of film for every 15 m of weld is the floor, and a supplier offering less is not offering Class 5. Second, UW-51 and UW-52 have different acceptance limits, so a Class 5 joint is not simply a Class 1 joint examined less often; the film is judged against a different clause.

Heat treatment and the “HT” stencil

Unless the order states otherwise, all pipe is furnished heat-treated per Table 2, which for the general case specifies 1900 °F [1040 °C]. When a final heat-treatment temperature below 1900 °F [1040 °C] is agreed, clause 6.3.2.1 requires each length to be stencilled with the actual final temperature followed by the suffix HT. That stencil is your audit trail: it tells an inspector what the pipe actually saw, not what the purchase order assumed.

For stabilised grades — 321, 321H, 347, 347H, 348 — Supplementary Requirement S5 adds a stabilisation heat treatment after the initial solution anneal, at a temperature below the annealing temperature and as agreed between purchaser and manufacturer. S6, when invoked, requires passing intergranular corrosion testing to ASTM A262 Practice E, and for titanium- or columbium-bearing grades S6 may make S5 necessary to comply.

A358 vs A312 vs A778: which specification do you need?

ASTM A358ASTM A312ASTM A778
Welding routeElectric fusion welded from plateSeamless, straight-welded, or heavily cold-workedWelded, general corrosion service
Typical size bandNPS 8 and up in commercial practiceFull NPS range, with welded product generally below the large-diameter bandLarge diameter, light to moderate wall
Class systemYes — Classes 1 to 5No class systemNo class system
GovernsHigh-temperature and corrosive service, with radiography options priced inGeneral corrosive and high-temperature service; the default stainless pipe specGeneral corrosion service where pressure rating is not the driver
Practical useWhen the project needs a declared weld class and RT coverageWhen the project needs a standard mill product at any sizeWhen the project needs large diameter at low pressure — ducts, stacks, drains

In plain terms: A312 answers “what is this pipe made of and how was it welded”. A358 additionally answers “how thoroughly was the weld inspected, and who signed off on that choice”. A778 answers “can you get me a large-diameter welded pipe for general service without a pressure-code paper trail”. Large-diameter thick-wall pressure work usually lands on A358; large-diameter thin-wall ducting usually lands on A778; anything that must be seamless lands on A312.

How to write an A358 purchase order

Most order disputes on A358 come from four fields left blank. Fill these and the specification does the rest:

  1. Class — state Class 1, 2, 3, 4 or 5 explicitly. Never write “A358” alone and expect a class.
  2. Grade and heat treatment — grade per Table 1, plus whether standard 1900 °F [1040 °C] anneal applies or a lower temperature is agreed (which then requires the HT stencil).
  3. Size basis — outside diameter and wall thickness. Above NPS 24, wall thickness is a project decision, not an ASME B36.19 schedule value; write the number you want, or write “per drawing”.
  4. Supplementary requirements — if you need S5 stabilisation or S6 intergranular testing, say so. They are optional by definition.
  5. Examination and documentation — confirm hydrostatic testing per A999/A999M (clause 15.2, with the 15.3 purchaser option noted), and specify the certificate: EN 10204 3.1 mill test certificate, plus third-party inspection if the project requires it.

What Shiwang supplies under A358

Shandong Shiwang Stainless Steel Pipe manufactures EFW stainless pipe under ASTM A358/A358M, with the weld class declared on the certificate rather than implied:

  • Outside diameter: up to 5000 mm, built as longitudinal JCOE sections and completed by circumferential welding where the diameter exceeds single-section capability.
  • Wall thickness: 6 mm to 80 mm on thick-wall product; thinner sections available on the thin-wall line.
  • Grades: 304/304L, 316/316L, 321, 310S, 2205 duplex as standard; 904L, Hastelloy, Inconel and titanium on request.
  • Classes: Class 1, 3, 4 and 5 supplied; Class 2 on request where the project accepts no radiography.
  • Examination: 100 percent RT or UT on Class 1, 3 and 4 seams, spot RT to the 300 mm / 15 m rate on Class 5, hydrostatic testing, PMI, dimensional and roundness checks.
  • Documentation: EN 10204 3.1 mill test certificate, chemical and mechanical reports, weld maps, heat-treatment records including HT stencilling where applicable, and SGS, BV or TUV third-party inspection on request.

Related product pages: extra-large diameter stainless steel welded pipe, large-diameter thick-wall welded pipe, and large-diameter thin-wall welded pipe. For dimension tables across the full large-diameter range, see the large-diameter stainless steel pipe size table.

FAQ

Which A358 class should I specify for a pressure application?

Class 1 or Class 3. Both require complete radiography of every welded joint, judged to UW-51. Class 1 gets you a double-welded seam; Class 3 gets you a single-welded seam with full RT. The choice between them is usually driven by wall thickness, welding position on the shell, and whether the purchaser’s specification names one of them. Class 5 is the cost-reduced option with defined spot coverage, and Class 2 has no radiography at all, so neither belongs on a pressure line without a specific engineering justification.

Is Class 5 an autogenous weld?

No. Class 5 is double welded with filler metal in all passes and spot radiographed. The autogenous exception in A358 belongs to Class 4, where the weld pass exposed to the inside surface may be made without filler metal under clauses 6.2.2.1 and 6.2.2.2. Any supplier describing Class 5 as filler-free is quoting from a secondary summary, not the standard.

What exactly does “spot radiographed” mean in Class 5?

Clause 16.2 sets the minimum at 12 in. [300 mm] of radiograph per 50 ft [15 m] of weld, examined to UW-52. It is a coverage rate, not a random sample by convenience. On a 12 m shell with two circumferential seams, that translates into a defined minimum film length per seam, and the location of the spot is agreed with the inspector.

Do I need to specify heat treatment separately?

Not for the standard case — Table 2 applies automatically at 1900 °F [1040 °C]. You do need to specify it when you want a different final temperature, in which case the HT stencil requirement under 6.3.2.1 applies, and when you want S5 stabilisation for 321, 321H, 347, 347H or 348.

Can A358 pipe be supplied above NPS 24?

Yes. The specification places no size restriction, and commercial practice is simply “NPS 8 and larger”. What changes above NPS 24 is the dimensional basis: ASME B36.19 schedules stop being meaningful, so wall thickness is written as a project value or per drawing, and the weld class plus RT coverage become the primary quality statement on the order.

What documentation should arrive with an A358 shipment?

At minimum, an EN 10204 3.1 mill test certificate covering chemistry and mechanical properties, the declared class, heat-treatment records, and radiographic reports for Class 1, 3, 4 and 5. Weld maps, PMI results, hydrostatic test records and third-party inspection reports are added when the order calls for them.

Request a quote with the class, grade and size clearly stated — we will confirm the RT coverage and documentation against your project specification before production.

Need a quote on a specific size?

Send the five parameters that drive the price: outside diameter, wall thickness, grade, length per section, and total quantity. We reply within one working day with a technical-commercial offer, including the proposed welding sequence and inspection plan.